A tensile result is only as good as the specimen. Nicked edges start tears in rubber and film, uneven width throws off stress calculations, and a poorly machined metal specimen may break outside the gauge length. This guide covers the main ways to make test specimens: cutting dies, punch presses, machining and marking, and how to choose between them.

Methods at a Glance

MethodMaterialsProsLimits
Cutting die + arbor pressRubber, film, thin plastic, foam, fabric, leatherFast, consistent, low costThin, soft materials only
Cutting die + pneumatic or hydraulic pressSame, higher volume or thicker sheetVery repeatable, less operator effortHigher cost
Punch press for metalThin sheet metalFast for sheetEdge condition must meet the method
CNC machiningMetals, rigid plastics, compositesAny shape, tight tolerancesSlower, needs a machine shop
Injection moldingPlasticsStandard specimens direct by moldingNeeds molds and molding press

Cutting Dies

A die is a sharp steel blade bent to the specimen outline. Pressing it through a sheet cuts a specimen to the exact dimensions of the standard, such as ASTM D412 dumbbells, ASTM D624 tear specimens and ASTM D638 Type IV plastics. Two common constructions:

  • Hardened steel dies: machined out of solid steel and hardened. They hold their edge longest and are the choice for high volume and abrasive compounds.
  • Ribbon (rule) steel dies: steel rule bent to shape and set in a holder. Lower cost and quick to make, but the edge wears sooner.

Video: Hardened steel vs ribbon steel cutting dies

Browse ASTM cutting dies and hardened steel dies.

Common Dies by Standard

StandardSpecimenMaterial
ASTM D412Dumbbell, Die C most commonRubber and elastomers
ASTM D624Die C right-angle, trouser or crescentRubber tear
ASTM D638Type IV and Type V dumbbellsThin plastic sheet
ASTM D1708Microtensile dumbbellPlastics
ASTM D1004Right-angle tearFilm and sheeting
ASTM D882Straight strip (cutter, not die)Film

Many ISO and DIN specimens have close equivalents with slightly different dimensions, so order dies to the exact standard you test to. See ASTM vs ISO equivalents.

Presses for Die Cutting

A manual arbor press handles most rubber and film cutting. Higher volume or thicker material calls for a pneumatic or air-hydraulic press, which applies the same force on every stroke.

Video: How to use an arbor press for ASTM and ISO sample cutting

Video: Air-hydraulic press for cutting samples

Good Die-Cutting Practice

  1. Cut on a cutting pad that is flat and not grooved by earlier cuts.
  2. Cut in the direction the standard specifies, with and across the grain or machine direction as required.
  3. Keep the die square to the sheet so edges are perpendicular.
  4. Use one firm stroke; do not rock the die.
  5. Inspect edges under magnification for nicks and tears; discard bad specimens.
  6. Measure thickness and width in the gauge section for every specimen.
  7. Sharpen or replace the die when edges start to show burrs or nicks.

Video: How to sharpen ASTM and ISO cutting dies

Machined Specimens

Metals, rigid plastics and composites are usually machined. Standards such as ASTM E8 specify dimensions, tolerances, fillet radii and surface finish. Machining marks across the gauge length can start cracks, so finish passes should run lengthwise. For high-volume metal labs, dedicated specimen preparation tools speed this up.

Video: ASTM E8 sample preparation tool for metal specimens

Measuring Specimens

Stress is force divided by area, so every error in width or thickness goes straight into the result. Measure each specimen in the gauge section, at several points, with an instrument suited to the material: a dial or digital micrometer with the foot size and pressure the method specifies for rubber and film, calipers or a micrometer for metals. Record the minimum cross-section unless the method says otherwise. Soft materials compress under a heavy micrometer foot, which reads thin and inflates the stress.

Sheet Metal and Impact Specimens

Thin sheet metal can be blanked with a punch press, but sheared edges are work-hardened and can lower elongation, so many metals methods require machined or finished edges. Charpy impact specimens need a precisely machined notch; a notch broaching machine cuts it to the standard profile. See the ASTM E23 guide.

Marking Gauge Length

Elongation needs marks at a known spacing. Ink or scribe marks work for manual measurement; video extensometers use high-contrast dots or lines, applied consistently with a marking tool.

Conditioning

Plastics, rubber, paper and textiles absorb moisture and change with temperature. Most methods require conditioning at a set temperature and humidity for a set time before testing. Record the conditioning with the results.

Related Guides

Frequently Asked Questions

How are tensile test specimens made?

Thin, soft materials are die-cut with a cutting die and press. Metals, rigid plastics and composites are machined, and many plastics are injection molded directly to standard dimensions.

What is the difference between hardened steel and ribbon steel dies?

Hardened steel dies are machined out of solid steel and keep their edge much longer. Ribbon steel dies are bent steel rule; they cost less but wear sooner.

How often should a cutting die be sharpened?

When cut edges start to show burrs, nicks or tearing. High-volume labs inspect specimen edges every shift.

Why do specimen edges matter so much?

Nicks act as notches. In rubber and film they start tears that cause early, low breaks and scattered results.

Do specimens need conditioning before testing?

Many plastics, rubber, paper and textile methods require conditioning at a set temperature and humidity for a set time before testing.