ASTM D638 Tensile Testing of Plastics: Specimen Types, Dies, Grips, Extensometers and Procedure
Created at : Oct 24, 2026ASTM D638 is the tensile test for plastics. Resin suppliers publish tensile strength, modulus and elongation to it, molders check incoming material against it, and design engineers use its numbers in every plastic part calculation. It is also the test most labs set up first when they buy a universal testing machine for plastics. This guide covers what D638 measures, the five specimen types and how to cut them, the grips, test speeds, extensometers, the step-by-step procedure, the calculations, the common mistakes, and the equipment list for a complete D638 setup.
Need flexural properties as well as tensile? The three-point bend method for plastics, with its speed table, deflection measurement options and calculations, is covered in our ASTM D790 complete guide and walkthrough.
Testing rubber or a soft thermoplastic elastomer rather than a rigid plastic? Those materials use ASTM D412, not D638; see our ASTM D412 complete guide and walkthrough.
Video: ASTM D638 plastics tensile testing grip
What ASTM D638 measures
- Tensile strength: the maximum stress the specimen carries, or the stress at yield for materials that yield before they break.
- Tensile modulus of elasticity: the slope of the stress-strain curve in its initial linear region, which needs an extensometer.
- Yield strength and yield strain for ductile plastics that show a yield point.
- Elongation at yield and at break, reported as percent strain.
- Poisson’s ratio, when transverse strain is measured as well as axial.
- Secant modulus for plastics with no linear region.
D638 applies to rigid and semi-rigid plastics thicker than 1 mm. Thin film and sheeting under 1 mm are tested to ASTM D882 instead, and small or scarce material to ASTM D1708 micro-tensile. Rubber and elastomers use ASTM D412. The international equivalent is ISO 527-2, which uses similar but not identical specimens, so results should not be mixed without checking.
The five specimen types
The standard specimen is a flat dumbbell. The wide ends sit in the grips and the narrow gauge section in the middle is the part that stretches and breaks. D638 defines five types; the choice depends on material thickness, how much material you have and how it was made.
| Type | Overall length | Gauge section width | Gauge length | Thickness | When to use it | Cutting die |
|---|---|---|---|---|---|---|
| Type I | 165 mm (6.5 in.) | 13 mm (0.50 in.) | 50 mm (2.0 in.) | 7 mm or less | The default for rigid and semi-rigid plastics; injection molded or die cut out of sheet | D638 Type I die |
| Type II | 183 mm (7.2 in.) | 6 mm (0.25 in.) | 50 mm (2.0 in.) | 7 mm or less | Materials that fail outside the gauge section as Type I; narrower gauge concentrates failure | D638 Type II die |
| Type III | 246 mm (9.7 in.) | 19 mm (0.75 in.) | 50 mm (2.0 in.) | 7 to 14 mm | Thick materials; the only type for specimens over 7 mm | D638 Type III die |
| Type IV | 115 mm (4.5 in.) | 6 mm (0.25 in.) | 25 mm (1.0 in.) | 4 mm or less | Comparing materials of different rigidity, and thin sheet; also matches ISO 527 Type 1BA geometry | D638 Type IV die |
| Type V | 63.5 mm (2.5 in.) | 3.18 mm (0.125 in.) | 7.62 mm (0.30 in.) | 4 mm or less | Limited material, specimens cut out of parts, and exposure or aging studies; same shape as ASTM D1822 Type L | D638 Type V die |
Type I is used in the great majority of data sheets. If you are generating data to compare with a supplier’s, match their specimen type, because results differ between types even for the same material.

Making the specimens
Specimens are injection molded in a D638 cavity, machined, or die cut. Molded specimens are the reference for resin data; molding conditions, gate location and orientation all affect the result, so they are recorded. Machined specimens are cut with a router template or CNC and the gauge edges polished, since a scratch starts a crack. Die cutting is the fast route for sheet, film and softer plastics: one stroke on a press gives a finished specimen with no edge finishing.
- Hardened steel dies are machined and ground tool steel; they cut rigid and semi-rigid plastics up to several millimetres thick and keep their edge for years.
- Ribbon steel dies use a thin steel blade bent to the dumbbell outline; they cost less and suit film, thin sheet, foam and softer materials.
- Dies are used in an 8 kN hand press or 17 kN arbor press over a cutting board. Cut in one steady stroke; a slow or double cut leaves a ragged edge.
- Inspect gauge edges before testing. Nicks and whitening at the edge lower the strength and elongation.
Video: Hardened steel vs ribbon steel cutting dies for ASTM specimens
Video: Sample molding trays for casting ASTM specimen sheets
Grips
The grip has one job: hold the tab ends without letting the specimen slip or break in the jaws. Rigid plastics are usually held in wedge grips, which tighten as load rises, or in pneumatic grips, which clamp with the same force on every specimen and speed up high-volume testing. Serrated jaw faces suit rigid materials; rubber-coated or smooth faces protect soft or thin ones. Grip the full width of the tab, align the specimen on the load axis and set the grip separation to the value the standard gives for the specimen type, 115 mm for Type I. A failure in the grip or at the tab radius is not a valid result.


Test speed
D638 sets the crosshead speed by specimen type and material, with the aim that rupture happens in 30 seconds to 5 minutes. The common speeds are 5 mm/min (0.2 in./min) for rigid Type I, II and III specimens, 50 mm/min (2 in./min) for semi-rigid and for Type IV, and 500 mm/min (20 in./min) for very ductile materials and for Type V. Modulus is normally measured at the slowest speed for the material and the test can then be sped up after the extensometer is removed, which the standard allows. Speed changes the result for most plastics, so it is always reported.
Measuring strain: extensometers
Crosshead travel includes the stretch of the grips, the tabs and the load frame, so a modulus based on crosshead travel is wrong, usually by a wide margin. D638 requires an extensometer for modulus, and it is the biggest single accuracy decision in a plastics lab.
| Option | How it works | Best for | Limitation |
|---|---|---|---|
| Clip-on extensometer | Knife edges clipped to the gauge section | Modulus on rigid plastics; lowest cost | Must be removed before break on brittle or high-elongation materials; knife edges can start cracks in soft plastics |
| High-elongation clip-on | Long-travel arms clipped to the specimen | Ductile plastics to 100 percent and beyond | Still contacts the specimen; one gauge length per model |
| 2D video extensometer (ONE M1, M5) | Camera tracks gauge marks | Any specimen type, modulus and elongation to break, no contact | Needs marks or targets; a marking tool keeps them consistent |
| 3D DIC extensometer (Vector U70) | Stereo cameras track the surface pattern | Thin and small specimens, strain to fracture, out-of-plane movement ignored | Higher cost than 2D |
| Biaxial 3D extensometer (B80) | Axial and transverse strain at once | Poisson’s ratio | As above |
Video: ASTM D638: measuring elongation with a video extensometer
Video: Automatic balanced extensometer on plastics
Video: Gauge length marking tool for video extensometers
For more on choosing between contact and non-contact strain measurement, see our clip-on extensometer buying guide.
Step-by-step ASTM D638 procedure
- Condition the specimens at 23 °C and 50 percent relative humidity for at least 40 hours, as ASTM D618 requires, unless the material specification says otherwise. Many plastics, nylon above all, change properties with moisture.
- Measure width and thickness at the center and both ends of the gauge section, and use the average area. A micrometer with the right contact pressure matters on soft plastics.
- Set the grip separation for the specimen type and mount the specimen centered and aligned.
- Attach the extensometer or apply gauge marks, and zero force and strain.
- Run the test at the specified speed, recording force and strain. Remove a clip-on extensometer after the modulus region if the material is brittle or stretches far.
- Continue to rupture, or to the strain limit your specification sets.
- Check the failure location. Breaks in the gauge section are valid. Breaks at the tab radius or in the grip are discarded and replaced; a pattern of tab failures means the specimen type or grip faces need changing.
- Test five specimens per sample as a minimum, or more for anisotropic materials, and report mean and standard deviation.
Calculations
| Result | Calculation | Units |
|---|---|---|
| Tensile stress | Force divided by original cross-sectional area of the gauge section | MPa (psi) |
| Tensile strength | Maximum stress reached, or stress at yield if that is higher than at break | MPa (psi) |
| Yield strength | Stress at the first point of zero slope on the stress-strain curve | MPa (psi) |
| Elongation at break | Change in gauge length at rupture divided by the original gauge length, times 100 | percent |
| Modulus of elasticity | Slope of the initial linear part of the stress-strain curve, with the toe region corrected out | MPa (psi) |
| Secant modulus | Stress divided by strain at a stated strain, for curves with no linear region | MPa (psi) |
| Poisson’s ratio | Negative of transverse strain divided by axial strain in the linear region | none |
Worked example: a Type I specimen 13.0 mm wide and 3.2 mm thick has an area of 41.6 mm². A maximum force of 2,080 N gives a tensile strength of 2,080 / 41.6 = 50.0 MPa. If the extensometer reads 1.25 mm over a 50 mm gauge length at break, elongation at break is 2.5 percent.
Common mistakes
- Modulus taken off crosshead travel. It can be half the true value. Use an extensometer.
- Skipping conditioning. Dry nylon and wet nylon are different materials.
- Wrong speed for the material. Faster tests give higher strength and lower elongation in most plastics.
- Edge damage on die-cut or machined specimens, which fails early.
- Mixing specimen types or comparing molded with cut specimens.
- Counting tab failures. Only gauge-section breaks are valid.
- A load cell that is too big. A 50 kN cell reading 500 N is at 1 percent of range; use a cell sized to the material, see our load cell guide.
Equipment for a complete D638 setup
| Item | What to look for | Our options |
|---|---|---|
| Testing machine | Enough force for your strongest material with margin, crosshead travel for ductile plastics, speed range 1 to 500 mm/min | 5 kN, 10 kN and 25 kN benchtop machines; see the cost guide |
| Load cell | Sized so typical tests use 10 to 80 percent of range | Load cells |
| Grips | Wedge or pneumatic, serrated or coated faces, 115 mm separation for Type I | Wedge grips, pneumatic grips |
| Extensometer | Class B-1 or better for modulus; video or 3D for elongation to break | Clip-on, video, 3D DIC |
| Specimen preparation | Dies for each type and a press, or a mold | Cutting dies, hand press |
| Conditioning | 23 °C and 50 percent RH; chamber for tests at temperature | Environmental chambers; see the chamber guide |

Video: Automated material testing system for plastics
Related plastics tests
- ASTM D882 tensile properties of thin plastic sheeting and film
- ASTM D1708 micro-tensile specimens when material is limited
- ASTM D695 compressive properties of rigid plastics
- ASTM D790 and D6272 flexural properties
- ASTM D2990 tensile and compressive creep
- ASTM D256 Izod and D6110 Charpy impact resistance
Frequently asked questions
What is ASTM D638?
The standard test method for the tensile properties of plastics. A dumbbell specimen is pulled at a set speed on a universal testing machine to measure tensile strength, modulus, yield and elongation.
Which ASTM D638 specimen type should I use?
Type I for most rigid and semi-rigid plastics up to 7 mm thick. Type III for thicker material, Type IV for thin sheet and comparisons between materials, Type V when material is limited, Type II when Type I breaks outside the gauge section.
What test speed does ASTM D638 use?
It depends on the specimen type and material: 5 mm/min for rigid Type I to III specimens, 50 mm/min for semi-rigid materials and Type IV, 500 mm/min for very ductile materials and Type V. The target is rupture in 30 seconds to 5 minutes.
Do I need an extensometer for ASTM D638?
Yes, for modulus and accurate elongation. Crosshead travel includes grip and frame compliance and gives modulus values that are far too low.
What size testing machine do I need for plastics?
Most plastics fail below 5 kN in a Type I specimen; glass-filled grades can reach 10 kN. A 5 to 25 kN benchtop machine with a load cell sized to the material covers nearly every case.
What is the difference between ASTM D638 and ISO 527?
They are similar methods with different specimen dimensions and some differences in speed and modulus calculation. ISO 527-2 Type 1A is close to D638 Type I and Type 1BA to Type IV, but results should not be assumed interchangeable.
Can I die cut ASTM D638 specimens?
Yes. Hardened steel or ribbon steel dies in a hand or arbor press cut sheet, film and softer plastics cleanly. Rigid thick plastics are usually molded or machined.
Get a quote
Interested in an immediate price quote or an application discussion? Email christhomas@universalgripco.com or frank@universalgripco.com, or call or text us at 978-882-1480. Tell us the plastics you test, the specimen type and the properties you need, and we will recommend a machine, grips, extensometer and dies with a firm price.